AWS D1.1:2025 · Tabla 5.11 · Categoría A

Precalentamiento de A36 para SMAW (non-low-hydrogen) — 1-1/2" to 2-1/2"

Temperatura mínima de precalentamiento e interpaso para A36 soldado con SMAW (non-low-hydrogen) en espesor 1-1/2" to 2-1/2", según AWS D1.1:2025 Tabla 5.11.

Basado en AWS D1.1:2025 Tabla 5.11 — cada valor trazado a la cláusula.

Temperatura Mínima de Precalentamiento e Interpaso
225°F / 110°C
Categoría A
Proceso SMAW no bajo hidrógeno
AWS D1.1:2025 Tabla 5.11, §5.7
Herramienta de referencia. Verificar contra la edición aplicable al proyecto y WPS aprobada por el Ingeniero.

SMAW (Non-Low-Hydrogen)

Non-low-hydrogen SMAW (E6010/E6011) uses cellulosic electrodes with higher hydrogen potential, assigned to Category A in Table 5.11.

For common structural shapes and plate, non-low-hydrogen SMAW with E6010 or E6011 excels at root passes on open-root groove welds where burn-through control matters. Vertical-up technique with a slight weave keeps the puddle manageable. Rod consumption runs about 10-12 electrodes per pound of weld metal deposited. Electrode stubs should be no shorter than 2 inches to maintain adequate arc length control.

A36

ASTM A36 is the most commonly specified structural steel in North America, with a minimum yield strength of 36 ksi and 58-80 ksi tensile range. It appears in both Category A (non-low-hydrogen SMAW) and Category B (low-hydrogen processes) of Table 5.11. A36 is available as plate (up to 8" thick), W-shapes, channels, angles, and bars from virtually every domestic mill. Its moderate carbon content (0.26% max for shapes, 0.25% max for plate up to 3/4") and typical carbon equivalent of 0.35-0.42 give it good weldability across all prequalified processes. A36 plate thicker than 1-1/2" carries a slightly higher carbon limit of 0.29%, while plate from 3/4" to 1-1/2" stays at 0.25% max.

Por qué Este Precalentamiento para A36 con SMAW

Widely used structural carbon steel with 36 ksi yield and 0.26% max carbon. At this thickness, SMAW with non-low-hydrogen electrodes places the joint in Category A of Table 5.11. The minimum preheat of 225°F compensates for the higher diffusible hydrogen from cellulosic electrode coatings. The thicker the material, the longer hydrogen takes to escape the heat-affected zone, which is why preheat rises with thickness even for this common grade.

Aplicaciones Típicas de A36

Common in angle-to-gusset fillet welds, beam web clip angles, stiffener plates, base plate bearing connections, light bracing members, stair stringers, handrail posts, and miscellaneous steel fabrication. A36 plate is the default choice for connection elements such as shear tabs, moment end plates under 36 ksi demand, and simple beam-to-column seated connections. In retrofit and renovation, A36 angles and channels are standard for reinforcement brackets and framing infill. Typical shop drawing callouts include 3/8" and 1/2" A36 plate for gussets, 5/16" fillet welds on clip angles, and partial joint penetration groove welds on base plate stiffeners. A36 is so ubiquitous that most structural steel shops maintain permanent inventory in multiple thicknesses from 1/4" through 2" plate. Fillet weld sizes on A36 connections typically range from 3/16" minimum to 5/8" for heavy gusset-to-column welds, with E70XX electrodes providing significant overmatching strength.

Por qué el Precalentamiento Importa en 1-1/2" to 2-1/2"

Heavy plate with significant restraint and thermal mass — preheat is critical to maintain slow cooling for hydrogen escape.

Otros Aceros con SMAW (non-low-hydrogen) en 1-1/2" to 2-1/2"

AceroCategoríaPrecalentamiento
A53 Gr.BA225°F (110°C)
A106 Gr.BA225°F (110°C)

Prueba Diferentes Combinaciones

Usa la calculadora interactiva de precalentamiento para consultar cualquier combinación de acero, proceso y espesor de D1.1:2025 Tabla 5.11.

¿Cuál es el precalentamiento mínimo para A36 con SMAW en 1-1/2" to 2-1/2"?
Para A36 soldado con SMAW (non-low-hydrogen) en espesor 1-1/2" to 2-1/2", la temperatura mínima de precalentamiento es 225°F (110°C) según AWS D1.1:2025 Tabla 5.11, Categoría A. Esta es también la temperatura mínima de interpaso — la junta no debe enfriarse por debajo de 225°F entre pasadas.
¿Qué categoría de la Tabla 5.11 aplica a A36 con SMAW?
A36 soldado con SMAW (non-low-hydrogen) cae bajo la Categoría A en AWS D1.1:2025 Tabla 5.11. Proceso SMAW no bajo hidrógeno. En espesor 1-1/2" to 2-1/2", esta categoría requiere un precalentamiento mínimo de 225°F (110°C).
¿Por qué el precalentamiento es 225°F para A36 en 1-1/2" to 2-1/2"?
El precalentamiento de 225°F para A36 en 1-1/2" to 2-1/2" con SMAW (non-low-hydrogen) refleja la combinación de la templabilidad del acero y la restricción aumentada en este espesor. Un mayor precalentamiento reduce la velocidad de enfriamiento en la zona afectada por el calor, dando más tiempo al hidrógeno difusible para escapar.