Preheat Heat Input Fillet Weld Size Deposition Rate Carbon Equivalent
AWS D1.1:2025 · Table 5.11 · Category B

A709 Gr.50 Preheat for GMAW — over 2-1/2"

Minimum preheat and interpass temperature for A709 Gr.50 welded with GMAW at over 2-1/2" thickness, per AWS D1.1:2025 Table 5.11.

Minimum Preheat & Interpass Temperature
225°F / 110°C
Category B
Low-hydrogen SMAW, SAW, GMAW, or FCAW process
AWS D1.1:2025 Table 5.11, §5.7
Reference tool. Verify against project-applicable edition and Engineer-approved WPS.

GMAW (Gas Metal Arc Welding)

GMAW (MIG) feeds continuous solid wire with shielding gas — an inherently low-hydrogen process assigned to Category B in Table 5.11.

ER70S-6 wire at 0.035" or 0.045" diameter handles most structural work on common grades. Spray transfer at 250-350 amps provides high deposition for shop fillet welds. For thinner material under 1/4", short-circuit transfer at lower parameters reduces heat input. Gas flow rates of 35-45 CFH through a standard nozzle provide adequate shielding in typical shop environments without excessive turbulence.

A709 Gr.50

ASTM A709 Grade 50 is the standard bridge plate and shape grade with 50 ksi minimum yield and 65 ksi minimum tensile, commonly specified for highway bridge plate girder flanges, webs, floor beams, and cross-frames. It falls under Category B only in Table 5.11, requiring low-hydrogen welding processes. Chemistry mirrors A572 Gr.50 (0.23% max carbon, Nb/V microalloying) with CVN testing per AASHTO temperature zone requirements. A709 Gr.50 accounts for the majority of bridge steel tonnage in North America. Flange plate thicknesses routinely reach 2-3" on large plate girders, making preheat compliance at the upper Table 5.11 tiers a significant production consideration for bridge fabrication shops during cold-weather operations.

Why This Preheat for A709 Gr.50 with GMAW

Standard 50 ksi bridge plate for girders and cross-frames. This steel is prequalified only with low-hydrogen processes under Table 5.11, which is why it appears in Category B but not Category A. The 225°F minimum preheat with GMAW balances the steel's strength level and carbon equivalent against the controlled hydrogen input from the consumable. Non-low-hydrogen SMAW is not an option for this grade under D1.1 prequalified WPS.

Typical Applications for A709 Gr.50

Standard for highway bridge plate girder flanges, box girder webs, cross-frame angles, bearing sole plates, splice plates in bolted-welded connections, and composite deck studs. A709 Gr.50 is the baseline strength grade for most modern highway bridge design per AASHTO LRFD. Flange butt splices, web-to-flange continuous fillet welds, and bearing stiffener clips are the dominant weld types in girder fabrication. Girder flanges typically range from 3/4" to 3" thick with widths from 12" to 30", requiring extended preheat soak times on thicker flange splices. Bridge fabrication shops certified to AISC Major Steel Bridge category maintain dedicated preheat tracking logs for each flange splice throughout the production sequence. Web-to-flange fillet welds on plate girders often exceed 100 feet of continuous weld per girder, making SAW the standard process for these joints. Flange splice CJP groove welds undergo 100% UT examination per D1.5.

Why Preheat Matters at over 2-1/2"

The heaviest sections demand the highest preheat in Table 5.11. Multi-pass sequences require maintaining interpass temperature throughout.

Other Steels with GMAW at over 2-1/2"

SteelCategoryPreheat
A36B225°F (110°C)
A633 Gr.EC300°F (150°C)
A709 HPS70WC300°F (150°C)
A710 Gr.AC300°F (150°C)

Try Different Combinations

Use the interactive preheat calculator to look up any steel, process, and thickness combination from D1.1:2025 Table 5.11.

What is the minimum preheat for A709 Gr.50 with GMAW at over 2-1/2"?
For A709 Gr.50 welded with GMAW at over 2-1/2" thickness, the minimum preheat temperature is 225°F (110°C) per AWS D1.1:2025 Table 5.11, Category B. This is also the minimum interpass temperature — the joint must not cool below 225°F between passes.
What Table 5.11 category applies to A709 Gr.50 with GMAW?
A709 Gr.50 welded with GMAW falls under Category B in AWS D1.1:2025 Table 5.11. Low-hydrogen SMAW, SAW, GMAW, or FCAW process. At over 2-1/2" thickness, this category requires a minimum preheat of 225°F (110°C).
Why is preheat 225°F for A709 Gr.50 at over 2-1/2"?
The 225°F preheat for A709 Gr.50 at over 2-1/2" with GMAW reflects the combination of the steel's hardenability and the increased restraint at this thickness. Higher preheat slows the cooling rate in the heat-affected zone, giving diffusible hydrogen more time to escape before the steel transforms to a crack-susceptible microstructure.
How do I maintain preheat on very thick plate?
For material over 2-1/2”, preheat is typically applied with oxy-fuel torches or electric resistance blankets and monitored with contact thermometers or temp-sticks. The entire weld zone must reach the minimum temperature before welding begins, and interpass temperature is checked before each new pass. Insulating blankets help retain heat during pauses in multi-pass welding.