AWS D1.1:2025 · §7.11 · Table 5.11

Cold Weather Welding: D1.1 Requirements

When base metal temperature is below 32°F (0°C), D1.1:2025 requires 70°F (20°C) preheat on Table 5.11 entries marked footnote a (the 32°F [0°C] entries); others use their table minimum. Welding is prohibited below 0°F (−20°C) in the weld vicinity per §7.11.2. GMAW/GTAW/EGW/FCAW-G need wind shelter above 5 mph.

The 32°F Rule

D1.1:2025 Table 5.11 footnote a, which is attached only to the 32°F [0°C] entries, establishes the threshold: when base metal temperature is below 32°F (0°C), the base metal must be preheated to a minimum of 70°F (20°C) and the minimum interpass temperature must be maintained during welding. Entries without footnote a, such as the 50°F [10°C] entries, use their tabulated minimum instead.

For example, A36 with GMAW (Category B) normally requires no preheat for material up to 3/4 in thick. But if the beam is sitting in a laydown yard at 20°F in January, the welder must bring the joint area to at least 70°F before striking an arc. If the steel and process combination already requires a higher preheat (say 150°F for thick A992 with SMAW), use that value — such an entry carries no footnote a, so its tabulated minimum governs; the 70°F footnote applies only to the marked 32°F [0°C] entries.

In practice, this means carrying a rosebud torch or induction heater to the field in cold months. Measure with a contact pyrometer on the base metal — not the weld — per §5.7. Temperature-indicating crayons work but are less precise for this threshold check.

The 0°F Hard Stop

D1.1:2025 §7.11.2 prohibits welding when the temperature in the immediate vicinity of the weld is below 0°F [−20°C]. Its NOTE distinguishes this from the ambient environmental temperature and describes a heated structure or shelter that maintains the area adjacent to the weldment at or above that limit. Meeting base-metal preheat requirements alone does not establish compliance with this local environmental limit.

The prohibition exists because at extreme cold, base metal behavior changes: steel becomes more brittle, cooling rates become extreme regardless of preheat, and maintaining adequate interpass temperature becomes impractical. Hydrogen-induced cracking risk at these temperatures is severe.

Field tip: The 0°F limit is the temperature in the immediate vicinity of the weld, not the outside air and not the base metal temperature (that is a preheat question). If the air is −5°F but you have the joint inside a heated tent at 40°F, the enclosure meets the temperature condition in §7.11.2; the wet-surface, high-wind and personnel conditions still apply. Document the enclosure temperature in your daily report.

Wind and Shelter Requirements

D1.1:2025 §7.11.1 requires that GMAW, GTAW, EGW, and FCAW-G (gas-shielded flux-cored) not be done in a draft or wind unless a shelter reduces wind velocity in the vicinity of the weld to a maximum of 5 mph [8 km/h]. Wind disrupts the shielding gas envelope, causing porosity and contamination in the weld deposit.

Self-shielded processes (SMAW, FCAW-S) are less affected by wind because their shielding comes from flux decomposition rather than an external gas stream. However, strong wind still cools the weld and HAZ faster, which increases cracking risk in cold weather — so shelter benefits all processes.

Acceptable wind shelter includes temporary tarp windscreens or fully heated temporary structures. For GMAW, GTAW, EGW, and FCAW-G, §7.11.1 requires the shelter to reduce wind velocity in the vicinity of the weld to 5 mph [8 km/h] or less. In practice, a simple plywood or canvas screen on the windward side is often sufficient for field erection work.

Welding in Freezing Conditions — What D1.1 Actually Requires

To summarize, D1.1 sets cold-weather limits on two different temperatures: the base metal temperature (preheat) and the temperature in the immediate vicinity of the weld (§7.11.2):

Base metal at or above 32°F [0°C]: Apply the applicable Table 5.11 preheat and interpass requirements.

Base metal below 32°F [0°C]: Table 5.11 footnote a requires at least 70°F [20°C] preheat and maintenance of the minimum interpass temperature during welding on the 32°F [0°C] entries it marks. Entries without footnote a use their tabulated minimum. Protect gas-shielded processes from wind per §7.11.1.

Immediate weld vicinity below 0°F [−20°C]: Welding is prohibited under §7.11.2. A heated structure or shelter must maintain the vicinity at or above that limit; the other weather and personnel-exposure restrictions still apply.

Many fabricators and erectors also apply common-sense measures not explicitly required by D1.1: storing electrodes in heated ovens at the work station, warming filler metal, and using low-hydrogen processes (E7018, FCAW with H8 or better) to minimize cracking risk in cold conditions.

Field Tips for Winter Welding

In practice, this means: Start your shift by checking base metal temperature with a contact pyrometer before setting up. If the steel reads below 32°F and your Table 5.11 entry is a 32°F [0°C] entry marked with footnote a, fire up the rosebud and preheat the joint area plus 3 inches beyond in all directions. Verify 70°F minimum with the pyrometer, then maintain the minimum interpass temperature during welding. For any other entry, preheat to its tabulated minimum.

For multi-pass welds in cold weather, the biggest practical challenge is maintaining interpass temperature. The joint cools faster between passes when the surrounding steel is cold. Keep the heat source nearby and re-check temperature before each pass. Wrapping the joint area with ceramic blankets between passes helps retain heat.

Moisture management is the other critical factor. Cold steel below the dew point collects condensation. D1.1 §7.11.2 prohibits welding when surfaces are wet or exposed to rain or snow. In practice, preheat to 70°F also serves to drive off surface moisture — but inspect the joint visually before welding. Frost, ice, or visible moisture on the steel is a hard stop regardless of temperature readings.

Electrode storage matters more in cold weather. E7018 electrodes exposed to cold humid air absorb moisture faster than in dry conditions. Keep rods in a heated quiver or rod oven at the work station. If using FCAW, protect the wire spool from condensation with a sealed cover.

CWI Exam Tip

CWI Part C question pattern: A scenario describes welding structural steel with the base metal at 25°F. The question asks what minimum preheat applies. The answer is 70°F when the applicable Table 5.11 entry is a 32°F [0°C] entry marked with footnote a; for any other entry, the tabulated minimum for that steel, process and thickness applies. A common wrong answer is 32°F (that is the trigger temperature, not the preheat requirement). Another common wrong answer cites 0°F as the "no welding" threshold — which is correct as a fact but wrong as the answer to the preheat question.

Frequently Asked Questions

Yes, but with conditions. For the Table 5.11 entries marked with footnote a (the 32°F [0°C] entries), D1.1:2025 requires that when base metal temperature is below 32°F (0°C), the base metal must be preheated to a minimum of 70°F (20°C) and the minimum interpass temperature must be maintained during welding. Entries without footnote a use their tabulated minimum. Separately, §7.11.2 prohibits welding when the temperature in the immediate vicinity of the weld is below 0°F (−20°C).

D1.1:2025 §7.11.2 prohibits welding when the temperature in the immediate vicinity of the weld is below 0°F (−20°C); its NOTE says this is not the ambient environmental temperature. Preheating alone does not override it. The other weather and personnel-exposure restrictions in 7.11.2 still apply. Note that the threshold is 0°F, not 32°F.

D1.1:2025 §7.11.1 requires that GMAW, GTAW, EGW, and FCAW-G not be done in a draft or wind unless a shelter reduces wind velocity in the vicinity of the weld to a maximum of 5 mph [8 km/h]. This applies year-round but is especially critical in cold weather when wind chill accelerates cooling. The protection can be a temporary windscreen, tarp shelter, or permanent enclosure. SMAW and self-shielded FCAW-S are less wind-sensitive but still benefit from shelter in cold conditions.

Yes. Cold base metal acts as a heat sink, causing the weld and heat-affected zone to cool faster. Rapid cooling increases hardness and susceptibility to hydrogen-induced cracking, especially with high-carbon or high-strength steels. Cold weather also causes moisture condensation on the steel surface, which introduces hydrogen into the weld. D1.1 addresses cold weather through Table 5.11 footnote a on the 32°F [0°C] entries and the §7.11.1 wind shelter requirement.

If the base metal temperature is below 32°F (0°C), yes. For the Table 5.11 entries marked with footnote a (the 32°F [0°C] entries), D1.1:2025 requires preheating to 70°F (20°C) when the base metal is below freezing; entries without footnote a use their tabulated minimum. For A36 specifically, Table 5.11 Category A (SMAW non-low-hydrogen) normally requires no preheat for material up to 3/4 in thick. But if it is January and the steel is sitting at 15°F, you must preheat to at least 70°F before striking an arc.

Under D1.1:2025 §7.11.2, a heated structure or shelter may maintain the immediate vicinity of the weld at or above 0°F [−20°C]. Preheat is a separate requirement for the base metal. Wind protection under §7.11.1 (a shelter that reduces wind in the vicinity of the weld to 5 mph [8 km/h] for GMAW, GTAW, EGW, or FCAW-G) and the other §7.11.2 restrictions still apply. A blanket that keeps the base metal warm does not by itself show that the weld vicinity meets the 0°F condition.